    Screen printing adhesion test methods

    Date:2016/6/3 8:56:55 Hits:6317
     

        (1) the thumb test

    Condition: the experimental samples more than 5 PCS

    Experimental procedure: take sample, with your thumb on the picture of the printing, with 3 + / - 0.5 0 KGF force polishing the try 15 times back and forth.

    Experimental determination: products printing patterns and poor gap/break/ink adhesion, otherwise is unqualified.

         (2) 75% alcohol test

    Requirements: 1, the experimental sample 5 PCS more than 2, 3, 75% alcohol 4 white cotton gauze, 1.5 + / - 1.5 0 KGF system is provided

       Experimental procedures: 1.5 KGF system tied at the bottom of white cotton gauze, dipped in 75% alcohol, and then with white cotton gauze back and forth between 30 on the printing design (about 15 SEC).

       Experimental determination: products printing design shall have no loss/break/ink adhesion and poor gap, allowing yan.1.5 + / - 0.5 0 KGF system, light color, but not fuzzy printing pattern should be clear, otherwise is unqualified.

    (3) the 95% alcohol test

    Requirements: 1, the experimental sample 5 PCS more than 2, 3, 95% alcohol 4 white cotton gauze, 1.5 + / - 1.5 0 KGF system is provided

    Experimental procedures: 1.5 KGF system tied at the bottom of white cotton gauze, dipped in 95% alcohol, and then use white cotton gauze back and forth between 30 on the printing design (about 15 SEC)

    Experimental determination: products printing design shall have no loss/break/ink adhesion and poor gap, allowing yan.1.5 + / - 0.5 0 KGF system, light color, but not fuzzy printing pattern should be clear, otherwise is unqualified.

    (4) 810 tape test conditions: 1, the test sample 5 PCS more than 2, 810 tape experimental programs: the 810 tape completely paste on the silk screen printing, and then to the direction of the 45 degree Angle quickly pull up the tape, measured three times in a row.

    Experimental determination: products printing design gap/break.

    (5) 3 m600 tape test

    Conditions: 1, the experimental sample 5 PCS more than 2, 2, 250 tape test program: 3 m600 tape completely paste in screen printing, at an Angle of 45 degrees direction quickly pull up the tape.Only need to test again.

    Experimental determination: products printing design gap/break.

    (6) 250 tape test

    Conditions: 1, the experimental sample 5 PCS more than 2, 250 tape experimental programs: the 250 tape completely paste in screen printing, at an Angle of 45 degrees direction quickly pull up the tape, three times in a row.

    Experimental determination: products printing design gap/break.

    (7) gasoline wipe the test

    Requirements: 1, the experimental sample 5 PCS more than 2, 3 white cotton gauze, gasoline mixture (gasoline: 75% alcohol = 1:1) 4, 1.5 + / - 1.5 0 KGF system is provided

    Experimental procedures: 1.5 KGF system tied at the bottom of white cotton gauze, dipped in gasoline mixture, back and forth between 30 on the printing design (about 15 SEC)

    Experimental determination: products printing design shall have no loss/gap/break/ink and poor adhesion, allowing partial light, color but not fuzzy printing pattern should be clear, otherwise is unqualified.

    (8) hexane brush try testing

    Requirements: 1, the experimental sample 5 PCS more than 2, white cotton gauze hexane 3, 4, 1.5 + / - 0.5 0 KGF system

    Experimental procedures: 1.5 KGF system tied at the bottom of white cotton gauze, dipped in hexane solution, back and forth between 30 on the printing design (about 15 SEC)

    The experiment to determine: ditto a judgement

    Remark:

    1, 2, 4 as the general standard,

    3, 6 for SEB commonly used standard,

    5 for JARDEN commonly used standard,

    7 as SOLAC common standard,

    8 for SUNBEAM Australia are commonly used

     

      Home About UsProduct Special promotions Case  News  Train  Message  Contact Us
    Links: Huai'an OLAT Pad PrintingScreenPrinting(Northern distribution)
    Copyright::OLAT PRINTING MACHINERY INDUSTRY CO.,LTD.
    ADD:No.9?Zhangji?Road?Economic?Development?Zone,?Kunshan,?Jiangsu?Province
    TEL:0512-57068888 FAX:0512-57068800
    精品国产亚洲一区二区三区完整版_亚洲性色午夜无码一区二区三区_免费高清欧美亚洲视频_亚洲一区二区黄色网站
    1. 婷婷色制服中文字幕 | 中文字幕久久天堂一区二区 | 亚洲一级在线中文字幕 | 日韩一中文字幕在线 | 亚洲天堂在线观看视频 | 综合欧美日韩一区二区 |